Stainless Steel Physical Properties by Type
Density, elastic modulus, thermal expansion, conductivity, specific heat and electrical resistivity for ten stainless types, as published for BS EN 10088-1. Typical values for the grade type, not a promise about any part.
| Type (AISI) | EN grades covered | Density, kg/m³ | Modulus at 20 °C, GPa | Modulus at 400 °C, GPa | Mean CTE 20 to 100 °C, 10⁻⁶/K | Conductivity, W/(m·K) | Specific heat, J/(kg·K) | Resistivity, Ω·mm²/m |
|---|---|---|---|---|---|---|---|---|
| Ferritic | ||||||||
| 410S | 1.4000 | 7700 | 220 | 195 | 10.5 | 30 | 460 | 0.60 |
| 430 | 1.4016 | 7700 | 220 | 195 | 10.0 | 25 | 460 | 0.70 |
| 444 | 1.4521 | 7700 | 220 | 195 | 10.4 | 23 | 430 | 0.8 |
| Martensitic and precipitation hardening | ||||||||
| 410 | 1.4006 (410), 1.4005 (416), 1.4021 (420) | 7700 | 215 | 190 | 10.5 | 30 | 460 | 0.60 |
| 440 | 1.4112 (440B), 1.4122, 1.4125 (440C) | 7700 | 215 | 190 | 10.4 | 15 | 430 | 0.8 |
| 630 | 1.4542 (17-4 PH) | 7800 | 200 | 170 | 10.9 | 16 | 500 | 0.71 |
| Austenitic | ||||||||
| 304 | 1.4301 (304), 1.4305 (303), 1.4306 and 1.4307 (304L), 1.4541 (321), 1.4550 (347) | 7900 | 200 | 172 | 16.0 | 15 | 500 | 0.73 |
| 316 | 1.4401 (316), 1.4404 (316L) | 8000 | 200 | 172 | 16.0 | 15 | 500 | 0.75 |
| 6%Mo | 1.4547 (254 SMO) | 8000 | 195 | 166 | 16.5 | 14 | 500 | 0.85 |
| Duplex | ||||||||
| 2205 | 1.4462 (2205) | 7800 | 200 | n/a | 13.0 | 15 | 500 | 0.8 |
Source: British Stainless Steel Association, Ambient temperature physical properties of stainless steels to BS EN 10088-1, opened 25 October 2026. BSSA groups several EN grades under one AISI type, so 303, 304L, 321 and 347 share the 304 row, and 416 and 420 share the 410 row. The standard itself was not read; Annex E of BS EN 10088-1:2023 lists more grades. n/a: the source gives no 400 °C value for 2205.
| Type (AISI) | Density, lb/in³ | Modulus at 20 °C, 10⁶ psi | Mean CTE 20 to 100 °C, 10⁻⁶/°F |
|---|---|---|---|
| 410S | 0.278 | 31.9 | 5.8 |
| 430 | 0.278 | 31.9 | 5.6 |
| 444 | 0.278 | 31.9 | 5.8 |
| 410 | 0.278 | 31.2 | 5.8 |
| 440 | 0.278 | 31.2 | 5.8 |
| 630 | 0.282 | 29.0 | 6.1 |
| 304 | 0.285 | 29.0 | 8.9 |
| 316 | 0.289 | 29.0 | 8.9 |
| 6%Mo | 0.289 | 28.3 | 9.2 |
| 2205 | 0.282 | 29.0 | 7.2 |
Conversions: 1 kg/m³ = 3.6127 × 10⁻⁵ lb/in³; 1 GPa = 0.14504 × 10⁶ psi; a coefficient per kelvin divided by 1.8 gives the coefficient per °F. Rounded to the digits shown.
| Type (AISI) | Modulus of elasticity, GPa, at | Mean expansion between 20 °C and | |||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| 20 °C | 100 °C | 200 °C | 300 °C | 400 °C | 500 °C | 100 °C | 200 °C | 300 °C | 400 °C | 500 °C | |
| 430 | 220 | 215 | 210 | 205 | 195 | n/a | 10.0 | 10.0 | 10.5 | 10.5 | 11.0 |
| 410 | 215 | 212 | 205 | 200 | 190 | n/a | 10.5 | 11.0 | 11.5 | 12.0 | n/a |
| 630 | 200 | 195 | 185 | 175 | 170 | n/a | 10.9 | n/a | 11.1 | n/a | n/a |
| 304 | 200 | 194 | 186 | 179 | 172 | 165 | 16.0 | 16.5 | 17.0 | 17.5 | 18.0 |
| 316 | 200 | 194 | 186 | 179 | 172 | 165 | 16.0 | 16.5 | 17.0 | 17.5 | 18.0 |
| 2205 | 200 | 194 | 186 | 180 | n/a | n/a | 13.0 | 13.5 | 14.0 | n/a | n/a |
Source: British Stainless Steel Association, Elevated temperature physical properties of stainless steels, opened 25 October 2026, first table (BS EN 10088-1 data). n/a means the source gives no value. BSSA states it accepts no responsibility for the accuracy of the data it reproduces.
How to read the table
Density is a mass per volume at ambient temperature. It feeds weight and shipping estimates, and the spread inside the austenitic family is small: 7900 for 304 against 8000 for 316 is 1.3 percent.
Modulus is the elastic (Young’s) modulus. It falls as temperature rises: 304 goes from 200 GPa at 20 °C to 172 GPa at 400 °C in Table 3. A part that must keep its stiffness hot needs the hot value, not the room-temperature one.
Thermal expansion in this table is a mean over a stated range, not the value at one temperature. Table 1 uses 20 to 100 °C; Table 3 widens the range. Quoting a coefficient without its range is the commonest mistake: for 304 the figure is 16.0 over 20 to 100 °C and 18.0 over 20 to 500 °C. Worked example: a 100 mm length of 304 warmed by 50 K grows by 100 × 16.0 × 10⁻⁶ × 50 = 0.080 mm, while the same length of 430 grows by 100 × 10.0 × 10⁻⁶ × 50 = 0.050 mm.
Conductivity, specific heat and resistivity are 20 °C values. The 15 W/(m·K) of 304 and 316 is about half the 25 to 30 of 410S, 430 and 410, which matters when a part is heated unevenly. Resistivity is given in Ω·mm²/m, which equals micro-ohm metres.
Where sources disagree
A second table we opened, the SSINA design data page (opened 25 October 2026), lists 304 and 316 at 8.0 g/cm³ and 17.2 × 10⁻⁶/K over 20 to 100 °C, and 2205 at 7.85 g/cm³ and 13.0 × 10⁻⁶/K. Those differ from the 16.0 for 304 and 316 above, and the 7800 kg/m³ for 2205. Neither source is wrong: they follow different documents and rounding. Pick one source per calculation and say which on the drawing or the RFQ.
What to write on a drawing or RFQ
Name the material by standard and grade, such as 316L to ASTM A276 or 1.4404 to EN 10088-3, and leave the physical properties to the standard. If a modulus or an expansion coefficient is a design input, write the value, the temperature range and the source next to the note, and ask the supplier to confirm it for the product form being supplied. Do not ask a shop to guarantee a table value; these are reference figures for the alloy, and no shop is bound by them.
Related reading: distortion after machining and stress relief, the grade selection guide and the grade reference for composition and machinability. To have a drawing quoted by partner shops that cut stainless, send an RFQ.
Questions
Why does this page show 7900 kg/m3 for 304 when other sheets say 8000?
Sources round differently and quote different product forms. The BSSA table, which follows BS EN 10088-1, gives 7900 for 304 and 8000 for 316. The SSINA design table, taken from older handbooks, gives 8.0 g/cm3 for both. The gap is 1.3 percent. Use one source for the whole calculation and name it.
Do these figures apply to a machined part in any condition?
They are reference values for the grade type, quoted at 20 °C unless the column says otherwise. They are not measurements of your part. Cold work, heat treatment and product form can move some of them, so confirm any critical value with the supplier.
Which column matters most when a stainless part must hold size with temperature?
The thermal expansion column, read with the temperature range it was averaged over. An austenitic type such as 304 or 316 grows about 60 percent more per kelvin than a 430, from 16.0 against 10.0 in the same units over 20 to 100 °C.